Tensile Testing Plastics to ASTM D638 and ISO 527-2: Specimen Types, Grips, Extensometers and Speeds

Plastics look like the gentle end of a tensile laboratory. The forces are small, the frames are benchtop, and a molded dog bone needs no machining at all. Yet plastic results are among the hardest to reproduce from one lab to the next, because the number depends on more conditions than a metal test does: the speed, the temperature and humidity the specimen lived in, the way the specimen was made, and how the strain was measured in a window only a fraction of a millimeter wide.

Two standards cover most of this work. ASTM D638 is the reference in North America, and ISO 527-2, with the general rules of ISO 527-1, is used most widely elsewhere. ASTM itself notes that D638 and ISO 527-1 address the same subject matter but differ in technical content. This guide walks through where they differ and what each difference asks of the specimen, the grips, the extensometer and the frame.

In short
ASTM D638 or ISO 527-2: what is the real difference?
They cover the same subject with different specimens and a different speed rule. D638 offers five specimen types chosen to suit the material, while ISO 527-2 standardizes on one multipurpose specimen. ISO measures the modulus at 1 mm/min and then changes speed; D638 runs the whole test at one speed. Values for the same grade do not match directly.

What ASTM D638 Covers and Where It Stops

The current edition is D638-22. It covers the tensile properties of unreinforced and reinforced plastics in the form of standard dumbbell specimens, tested under defined conditioning, temperature, humidity and machine speed. Its range has two clear edges. It applies to material of any thickness up to 14 mm. Material thicker than that is machined down to fit. At the thin end, for sheeting and film under 1.0 mm, ASTM names ASTM D882 as the preferred method, and composites reinforced with oriented high-modulus fibers belong to ASTM D3039 instead.

Two lines in the scope matter more in practice than the rest. The first is that a material specification can modify the D638 procedure, and when it does, the specification takes precedence. A laboratory testing to a customer’s material sheet reads that sheet before it reads the standard. The second is that tensile properties of plastics vary with specimen preparation, speed and environment, and ASTM draws the consequence plainly: a material cannot be tested without also testing the way it was prepared, so every specimen in a comparison must be made the same way. That sentence is the reason the rest of this article spends as much time on the specimen as on the test.

ISO draws its boundaries in similar places. ISO 527-2 is written for rigid and semi-rigid thermoplastic and thermosetting molding, extrusion and cast materials, including short-fiber compounds, and it is not normally suitable for rigid cellular materials. Flexible films and sheets thinner than 1 mm go to ISO 527-3, and ISO 527-1 states that its definition of tensile modulus does not apply to films. In both systems, then, a product that drops below 1 mm changes standard, not only specimen.


Choosing the Dog Bone

D638 offers five specimen types, and ISO 527-2 offers essentially two. The difference reflects two philosophies. ASTM picks the specimen to suit the material and the amount available. ISO standardizes on one multipurpose specimen so that results from different laboratories line up.

ASTM D638 Types I to V

Type I is the default for rigid and semi-rigid plastics. Its narrow section is 13 mm wide and 57 mm long, it measures 165 mm overall, and it carries a 50 mm gauge length with the grips 115 mm apart. Molded specimens are typically 3.2 mm thick. Type II, with a 6 mm narrow section, is the next choice when a Type I does not break inside its narrow section. Type III is the thick-section specimen for material from 7 up to the 14 mm limit, at 246 mm overall. Type IV, with a 25 mm gauge length, is used for non-rigid plastics and when materials of very different rigidity have to be compared. Type V is the small one, about 63.5 mm overall with a 7.62 mm gauge, for cases where little material is available. The microtensile method, ASTM D1708, also uses a small specimen, but it reports strength and elongation only and is not used for modulus, and its scope points laboratories with little material to the D638 Type V instead. The small size has a cost of its own: a clip-on extensometer is hard to fit on a 7.62 mm gauge length, so Type V work tends to rely on non-contact strain measurement.

Before the first specimen is cut
Type I, 1A and 1B at One Scale
DRAWN TO SCALE, PLAN VIEW; TRANSITION RADII SCHEMATICASTM D638 Type Idefault for rigid and semi-rigid plasticsoverall 165 mm, narrow 13 x 57 mmgauge length 50 mmISO 527-2 type 1A (A1 since 2025)injection molded multipurpose specimenoverall 170 mm, narrow 10 x 80 mmgauge length 75 mmISO 527-2 type 1B (A2 since 2025)machined specimenoverall 150 mm, narrow 10 x 60 mmgauge length 50 mmgauge marksgrips 115 mm apart on all three
The three most common plastic dog bones drawn to the same scale. All three are gripped 115 mm apart, but the narrow section, the thickness and the gauge length differ, which is one reason a D638 value and an ISO 527 value for the same grade do not match.
Scroll the diagram sideways to see all of it.

ISO 527-2 Types 1A and 1B, Now A1 and A2

ISO 527-2 ties the specimen type to how the specimen is made. Type 1A is the directly injection molded multipurpose specimen and may also be used for compression molded specimens. Type 1B is the machined specimen. Both have a narrow portion 10 mm wide and a preferred thickness of 4 mm, and both are held with the grips 115 mm apart. Type 1A is 170 mm long with an 80 mm narrow portion, and its preferred gauge length is 75 mm, with 50 mm acceptable for quality control. Type 1B is 150 mm long with a 60 mm narrow portion and a 50 mm gauge length.

The 2025 edition of ISO 527-2 renamed the two types A1 and A2 to match ISO 20753, which now sets the multipurpose specimen. Most material data sheets, procedures and quotations still say 1A and 1B, so it is worth writing both names on a test request until the new ones are common.

Why the Two Specimens Do Not Give the Same Number

A Type I bar and a 1A bar differ in width, thickness and gauge length, and a plastic’s response depends on all three. ASTM notes that a change in thickness changes the ratio of surface to volume, and that for directly comparable results specimens should be of equal thickness. Molding history adds a further layer: injection molded and extruded material carries flow orientation, and ISO 527-2 asks for specimens to be taken both parallel and normal to the flow direction where the anisotropy matters. Before comparing a value from a D638 data sheet with one from an ISO data sheet, check the specimen, the thickness and the direction, not only the material name.

ASTM D638 Type I
Narrow section: 13 mm wide, 57 mm long
Gauge length: 50 mm
Thickness: typically 3.2 mm molded
ISO 527-2 Type 1A
Narrow portion: 10 mm wide, 80 mm long
Gauge length: 75 mm, 50 mm for quality control
Thickness: 4 mm preferred

Making the Specimen: Molded, Machined or Cut

ISO 527-2 prefers the injection molded multipurpose specimen and allows specimens to be machined, cut or punched from molded plates, or taken from cast or extruded plate. Its conditions are strict on the result rather than the route: all surfaces of the test specimen must be free of visible flaws, scratches or other imperfections, and flash is removed without damaging the molded surface. Two further sentences in the standard deserve attention. For reinforced plastics, specimens should not be machined to reduce their thickness unless it is unavoidable. And specimens with machined surfaces will not give results comparable to specimens with non-machined surfaces. A laboratory that switches from molded to machined bars mid-program has changed the test.

Molding carries variables of its own. ISO 294-1 sets out the general principles for injection molding thermoplastic test specimens and the mold designs for the multipurpose bar, and the interlaboratory tests behind it showed that the design of the mold is an important factor in the result. ASTM D3641 is the corresponding ASTM practice. Two laboratories molding the same grade in different tools can therefore see a difference that has little to do with the material.

When the specimen is machined, ISO 2818 is the reference. Its introduction makes the central point directly: machining influences the finished surfaces and in some cases the internal structure of the specimen, and because results depend strongly on both, exact definitions of the tools and machining conditions are needed for reproducible results. It allows dumbbells to be milled, names the parameters to report with them (cutting speed, feed speed, feed path and depth of cut), and asks that machined surfaces and edges be free of visible flaws when viewed under a low-power magnifier of about five times.

TensileMill CNC MICRO precision flat tensile and impact specimen preparation machine with its enclosure and coolant tank
The TensileMill CNC MICRO prepares flat specimens up to 8 in long from metal, plastic and composite sheet, machining both sides in one cycle without re-clamping. A D638 Type I at 165 mm and an ISO 1B at 150 mm both fit that length.

Research on edge quality supports that caution. A study of dumbbells cut from talc-filled polypropylene compared milling, laser cutting and water-jet cutting. Water-jet edges were the roughest and gave the lowest resistance to failure, and milling gave the best edge quality and the most repeatable results. The authors also noted that current standards do not say how specimens should be machined or set a limit on edge roughness. A separate study on printed polymer specimens found that removing an external notch raised the share of fractures inside the gauge length from 27 percent to 62 percent. Different materials, same lesson: the edge decides where the specimen breaks, and a break outside the narrow section is a result the standard does not accept.

Three checks before a machined plastic set goes to the frame
Look at the edge, not only the width. ISO 2818 asks for flaw-free edges under about five times magnification. A burr or a tool mark on the narrow section is a crack starter on a notch-sensitive polymer.
Keep the route fixed. Machined and molded surfaces do not give comparable results, so a comparison program uses one route for every specimen in it.
Record the direction. Plates carry flow orientation. Mark which way each blank was cut so the report can say parallel or normal to flow.

Conditioning comes before the test, whatever the route. D638 refers to ASTM D618, and the common Procedure A holds specimens at 23 °C and 50 percent relative humidity for at least 40 hours before testing, then tests in the same atmosphere. Polyamides, polyesters and polyurethanes take up water from the air, and their properties follow it, so a specimen machined with coolant or stored in an uncontrolled room needs its full conditioning time before it means anything. ISO testing refers to ISO 291 for its standard atmospheres. The material specification can override either.


Speed, Strain and the Modulus Window

The two standards treat speed differently, and it is the clearest practical difference between them. D638 runs the whole test at one speed chosen from its table. For rigid and semi-rigid materials on Types I to III that is commonly 5 mm/min, with 50 and 500 mm/min available for faster cases and non-rigid materials. Where neither the material specification nor the parties set a speed, laboratories describe the D638 rule as choosing the lowest speed that breaks the specimen within half a minute to five minutes, which usually means a preliminary test on a new material.

ISO 527 splits the test in two. For the tensile modulus on types 1A and 1B, ISO 527-2 sets 1 mm/min, roughly one percent strain per minute. Once the modulus range is passed, the test continues at the speed the material specification calls for, commonly 5 or 50 mm/min. A frame that runs ISO 527 changes speed during the test, and the software has to do it at a defined strain, not by hand.

Where the modulus is measured
A Window a Tenth of a Millimeter Wide
FIRST PERCENT OF A RIGID PLASTIC CURVE, SHAPE SCHEMATIC0 %0.25 %0.5 %0.75 %1 %strainstressISO 527-1 modulus window0.05 to 0.25 %HOW SMALL THE WINDOW IS0.2 % of a 50 mm gauge length= 0.1 mm0.2 % of a 75 mm gauge length= 0.15 mmISO 527-1 asks for about 1 micrometerof extensometer accuracy for modulus.Crosshead travel cannot resolve this.
ISO 527-1 takes the tensile modulus between 0.05 and 0.25 percent strain. On a 50 mm gauge length that whole window is 0.1 mm of extension, which is why the modulus needs an extensometer on the specimen and not the crosshead reading. The curve shape is schematic.
Scroll the diagram sideways to see all of it.

The modulus itself is where the precision is spent. ISO 527-1 defines the tensile modulus as the slope of the stress-strain curve between 0.05 and 0.25 percent strain, calculated either as a chord or as a least-squares regression over that interval. On a 50 mm gauge length, that 0.2 percent window is a change in length of 0.1 mm, and on a 75 mm gauge length about 0.15 mm. Measuring a slope reliably inside a tenth of a millimeter is why ISO 527-1 sets the extensometer accuracy for modulus at about one micrometer, and why a longer gauge length makes the job easier. D638 takes the modulus from the initial linear region of the curve, with toe compensation to correct the zero, and laboratories describe its requirement for modulus as an extensometer meeting ASTM E83 class B-2.

A worked example shows how tight that is. The same sources put the D638 limit for modulus at a strain error of 0.0002 mm/mm, which on a 50 mm gauge length is 0.01 mm. The ISO modulus window on that gauge is 0.1 mm, so the permitted error is a tenth of the whole measurement. For yield and elongation up to about 20 percent strain the requirement relaxes to E83 class C, and most clip-on extensometers are removed after yield or before the break. ASTM itself calls a true elastic limit in plastics debatable, and treats the initial-slope modulus as useful only if its arbitrary nature and its dependence on time and temperature are kept in mind.

Both standards agree on one thing: modulus is not taken from crosshead movement. The frame, the load cell and the grips all deflect under load, and on a plastic bar that deflection is not small compared with the specimen’s own stretch. A clip-on extensometer on the gauge length is the usual tool for rigid plastics. For soft, very ductile plastics that stretch far beyond a clip-on’s travel, long-travel or non-contact video extensometers are used, and our guide to extensometers goes through the types.

The rest of the procedure is familiar from metals but tighter. At least five specimens are tested for an isotropic material and ten for an anisotropic one, five in each direction. Width and thickness are measured at the center of the gauge length. The nominal cross-section is 41.6 mm² for a Type I bar (13 by 3.2 mm) and 40 mm² for a 1A bar (10 by 4 mm), and a thickness reading 0.1 mm off is about 3 percent of a 3.2 mm bar and 2.5 percent of a 4 mm bar, an error that passes straight into the stress and the modulus. A specimen that breaks at a flaw or outside the narrow section is discarded and replaced unless the flaw is what the test is studying, which brings the argument back to the edge. Our article on why tensile specimens break outside the gauge section covers the geometry side of that problem.

The report is where comparability is kept or lost. ISO 527-2 asks for the specimen type and the testing speed to be stated alongside the reference to the standard. A D638 report, as laboratories describe it, covers the preparation, the specimen type and dimensions, the conditioning, the number and direction of specimens, the test speed, the extensometer class and the edition of the standard. The edition is no longer a formality: since 2025 the same ISO bar can appear as 1A or A1, and a reader of an older report needs to know which document it followed. ASTM adds a final caution, that the data do not apply to load-time scales or environments widely different from those of the test.

What keeps a plastic tensile result comparable
  • A tiny modulus window: ISO 527-1 takes the modulus between 0.05 and 0.25 percent strain, which is 0.1 mm of extension on a 50 mm gauge length.
  • Strain comes from the specimen: neither standard takes the modulus from crosshead movement.
  • Thickness errors carry through: a reading 0.1 mm off is about 3 percent of a 3.2 mm bar, and it passes straight into the stress and the modulus.
  • Enough specimens: at least five for an isotropic material and ten for an anisotropic one.
  • Name the edition: since 2025 the same ISO bar can appear as 1A or A1.

Grips and Frames for Plastic Specimens

Plastics are notch-sensitive at the grip as well as at the edge. A jaw face aggressive enough for steel can bite into a polymer tab and start the break there, and a grip that loses force as the specimen thins under load lets it slip. The grip choice follows the material. For soft, thin or flexible plastics, pneumatic grips hold a constant, adjustable clamping pressure set for the material, so the force does not change as the specimen necks. Side-action grips with interchangeable smooth, serrated or rubber-coated faces suit rigid and semi-rigid bars. Self-tightening and eccentric roller grips, whose clamping force rises with the load, handle thin plastics and flexible strips. Our guide on how to choose tensile grips and fixtures explains the trade-offs in more detail.

The specimen geometry can help the grip. ISO 527-2 allows the tabs of a 1A bar to be extended, to 200 mm for example, when specimens slip, and it holds the initial grip separation at 115 mm within 1 mm, where published summaries of D638 give the Type I grip distance a tolerance of 5 mm either way.

TM-EML Series A single column benchtop universal testing machine for plastics tensile testing
The TM-EML Series A single-column benchtop frame covers 50 N to 5 kN, the force range most plastic dog bones need, and its page names ASTM D638 and ISO 527 among its typical tests.

The frame matters less for force than for control. A Type I bar of a rigid plastic breaks at forces that a benchtop frame handles easily, so capacity is rarely the limit. What counts is a load cell sized so the expected peak sits well inside its range, a crosshead that holds 1 mm/min steadily for the modulus stage and then changes speed on cue, and software that records force and extensometer strain fast enough to resolve the modulus window. As a rule of thumb from our own UTM guidance, choose a load cell where the expected peak load uses 10 to 70 percent of its range. The benchtop machine guide walks through the rest of that choice.

ISO 527-2 gives a useful sense of the data rate. For the modulus stage at 1 mm/min on a 1A bar with a 75 mm gauge length and 115 mm between the grips, it notes that recording strain at least 22 times a second is appropriate. The TM-EML frames control and sample at 1,200 Hz, so on these frames the limit is the extensometer’s resolution, not the data rate. For brittle grades, our frame guidance recommends a soft start and a low-force preload, and names rigid plastics that may fragment on failure as a reason for the optional interlocked safety enclosure.

How the speed runs
Two Stages or One
CROSSHEAD SPEED THROUGH ONE TEST, SCHEMATIC, HEIGHTS AND TIMES NOT TO SCALEISO 527-2modulus stage, then strength stagetimeASTM D638one speed for the whole testtime1 mm/minto past 0.25 % strain5 or 50 mm/min as the material standard setsbreakcommonly 5 mm/min for rigid Types I to IIIbreak
ISO 527-2 measures the modulus at 1 mm/min and then changes to the strength speed set by the material standard. ASTM D638 runs at one speed from its table, commonly 5 mm/min for rigid Types I to III. The time axis is schematic.
Scroll the diagram sideways to see all of it.
Plastics testing equipment
From the Dog Bone to the Modulus
A plastics program needs three things to agree: a specimen made the same way every run, grips that hold it without starting a break, and a frame that measures strain inside a window of a tenth of a millimeter.
TensileMill electromechanical universal testing machines for plastics tensile testing to ASTM D638 and ISO 527
Electromechanical Universal Testing Machines
The TM-EML series runs from a single-column 50 N to 5 kN benchtop frame to dual-column machines, and names ASTM D638 and ISO 527 among its typical tests. GenTest software comes with ASTM and ISO methods preloaded, and the frames support clip-on, laser and video extensometers.
Plastics and polymers
Control and sampling at 1,200 Hz
Installation, training and calibration
TensileMill grips and fixtures for plastic tensile specimens
Grips for Plastic Specimens
Pneumatic clamping grips with adjustable pressure for soft and flexible plastics, side-action grips with smooth, serrated or rubber-coated faces for rigid bars, and self-tightening and eccentric roller grips for thin plastics and films.
Rigid to flexible
Pressure set for the material
Interchangeable jaw faces
TensileMill CNC flat tensile specimen preparation machines for machining dog bone specimens from sheet
Machined Dog Bones from Sheet
The TensileMill CNC MICRO prepares flat specimens from metal, plastic and composite sheet or strip, both sides in one cycle, with positioning within 0.01 mm and an 18,000 rpm spindle. A free proof of concept on your own material is available before purchase.
Sheet and plate
Specimens up to 8 in long
Free proof of concept

If your laboratory machines plastic specimens from sheet, the fastest way to know whether a route gives clean, repeatable edges on your polymer is to cut a set and test it. Send us your material and the specimen type you need and we will prepare a sample set under our free proof of concept, so the edge quality can be judged on your own material before anything is bought.

Next step
Send us the polymer, the specimen type and the standard
Tell us which plastics you test, whether your customers ask for ASTM D638 or ISO 527, the specimen types and thickness you use, whether your specimens are molded or machined from sheet, and how many tests a shift runs. We will confirm the frame, the load cell, the grips and the extensometer setup, and if you machine your own specimens, prepare a sample set on your material.
Related machines
Equipment That Does This Work

RELATED TO STANDARDS

More standards can be added on-site with licensed TM Software, no specialist training required.

Your team can extend the machine to new test standards at any time using the machine's licensed TM Software, without CNC programming experience or outside help.

Have a tensile sample prep or testing question?