A reinforcing bar reaches the test laboratory in a different state from almost every other metal specimen: there is nothing to machine. The bar is pulled as it left the mill, ribs and mill scale included, and its stress is calculated on a nominal area. That moves the hard parts of rebar testing into the grips that hold a ribbed, scaled bar, the frame capacity for the largest sizes, the gauge marks punched on an uneven surface, and the reading of yield on bars that may or may not show a clear yield point.
ASTM A615/A615M is the product specification and sets what a carbon-steel bar has to achieve. ASTM A370 is the test method, with an annex for reinforcing bars, and where the two differ, the product specification controls. We do not reprint the A615 requirement tables here; the values that count are the ones in the edition your order names.
What ASTM A615 Asks of a Bar
The current edition is A615/A615M-26, updated in March 2026. It covers deformed and plain carbon-steel bars for concrete reinforcement, in cut lengths and coils, in Grade 40 [280], Grade 60 [420], Grade 80 [550] and Grade 100 [690], where the grade number is the minimum yield strength in ksi [MPa]. DOT procedures often cite the AASHTO twins instead, M 31 for A615 and T 244 for A370.
The specification calls for a heat analysis, a tension test reporting tensile strength, yield strength and elongation, a bend test, and a check of the deformations. The bend test needs its own equipment: the bar is bent around a pin whose diameter grows with bar size and passes if no cracks appear on the outside of the bend. A laboratory taking on A615 work has to plan for it separately from the tensile frame.
The edition matters, because the numbers have moved. A615-20 lowered the minimum tensile strength of Grade 60 to 80,000 psi and of Grade 80 to 100,000 psi, as CRSI reports, so both now match ASTM A706. In the 2009 edition tabulated by NIST, the Grade 60 minimum was 90 ksi. Elongation is set by bar size and grade and falls as the bar gets bigger: in that 2009 edition, Grade 60 needed 9 percent in 8 in. for #3 to #6 and 7 percent for #9 and larger. Grade 100, introduced in 2015, carries a warning in the standard itself: its specified tensile-to-yield ratio is 1.15, against 1.25 to 1.50 for the lower grades, which leaves less warning of failure after yielding, and its splices are expected to reach 115,000 psi.
A706 explains why designers care about the actual numbers a laboratory reports. It covers low-alloy bars with restricted chemistry, for controlled tensile behavior or better weldability. Its 2009 edition capped Grade 60 yield at 78 ksi and required tensile strength of at least 1.25 times the actual yield, while A615 set no maximum yield. For seismic frames and walls, ACI 318-11 allowed A615 Grade 60 only if the actual yield exceeded the specified value by no more than 18,000 psi and actual tensile over actual yield was at least 1.25. Those checks run on the laboratory’s measured values. The bar shows its certification in the deformations: S for A615, W for A706, both for dual grade.
The Specimen Is the Bar
Rebar tension and bend specimens are the full section of the bar as rolled. A draft specification on the A706 model, prepared for the ACI Foundation, says so directly, and every DOT and university procedure we drew on tests the bar the same way. Our article on preparing tensile specimens to ASTM A370 makes the same point: for rebar, the work moves from machining to the grips, the frame and the gauge marks. No specimen preparation machine is involved: turning a ribbed bar round would remove the surface being judged.
Nominal Area and the Weight Check
A deformed bar has no single diameter to measure, so its nominal dimensions are those of a plain round bar with the same weight per foot. A #5 bar is 0.625 in., 0.31 in.² and 1.043 lb/ft; a #8 is 1.000 in., 0.79 in.² and 2.670 lb/ft; a #11 is 1.410 in., 1.56 in.² and 5.313 lb/ft. Under A370 the tensile strength is the maximum load divided by that nominal area, and Delaware DOT calculates yield and tensile stress the same way.
Because the area comes from the weight, the weight is checked. Delaware DOT reports weight per foot for every rebar sample, and the ACI Foundation draft accepts a bar at 94 percent or more of nominal weight and never rejects one for being heavy. Dividing 2.670 lb/ft by the 0.785 in.² of a 1.000 in. circle gives 3.40 lb/ft per square inch of section, so measured weight divided by 3.40 is the actual area: for a #5, 1.043 / 3.40 = 0.307 in.², which rounds to 0.31. A bar at 94 percent of nominal weight still has its stress reported on the full nominal area, so it reports less than its steel carried. Weighing a measured length before the pull tells a light bar from a weak one.
Cutting, Straightening and Marking the Gauge
The structural laboratory at the University of Texas at Austin cuts bars to about 30 in., deburrs the cut and tests three samples per size. Delaware DOT takes two pieces of about 3 ft per size and heat, one for tension and one for bend. AASHTO’s mill audits require a flush-end cut with no torch, deburred ends, and coiled bar straightened as directed. The length has to fill both grips and leave free bar between each gauge mark and the nearest grip.
Coiling and straightening cold-work the bar and change the shape of its stress-strain curve, which matters when yield is read later, and Caltrans keeps any straightening of bent hoop ends outside the gauge marks. Delaware DOT marks the 8 in. gauge with a centre punch near mid-length, light, sharp marks spaced 8 in. within 1/16 in. The ACI Foundation draft places them on a longitudinal rib or in a clear space of the deformation pattern, never on a transverse deformation, and prefers light marks made with a bullet-nose punch, because deep ones indent the bar and may affect the result.
Gripping a Deformed Bar
Delaware DOT asks three things of a rebar grip: transmit the load axially, keep bending and twisting to a minimum, and hold the bar only outside the gauge length. Ribs and scale make the first two harder than on a smooth round. The UT Austin procedure solves it by size: flat grips for #3 and #4, with shims for #3 and alignment aids on the flat jaws, and vee grips from #5 upward in four ranges, 0.59 to 0.98 in. for #5 to #7, 0.98 to 1.57 in. for #8 to #11, 1.57 to 2.17 in. for #14 and 2.17 to 2.76 in. for #18, all 7 in. long. A vee face touches a round bar on four lines and centres it.
Our dual-action hydraulic wedge grips are built for this specimen, and their product page names rebar. In side-action mode the jaws close from both sides under hydraulic pressure set before the test; in wedge-action mode the jaws slide along an angled seat, so grip force rises with the load. Our wedge clamping grips use serrated or knurled faces on an internal wedge, in manual and hydraulic versions, with capacities exceeding 500 kN, and our hydraulic UTM grips take interchangeable jaw inserts.

Mill scale is the housekeeping problem rebar adds. The UT Austin procedure notes that a lot of scale falls onto the lower grips in every rebar test and has to be cleaned off so that it does not collect in the jaw mechanism. A slipping bar usually shows itself in the result: as our A370 preparation guide notes, it tends to report a low yield and a long elongation. Our guide on how to choose tensile grips and fixtures covers slippage and misalignment, and load-train alignment can be checked to ASTM E1012.
Mechanical splices need more room. A coupler test proposed for AASHTO asks for at least the splice length plus 16 bar diameters between the grips, and Caltrans for eight bar diameters plus 16 in. plus the coupler length. The TM-SHM frames list a maximum tension space of 520 to 1,200 mm depending on model, so coupler work is settled before the model is chosen.
Reading Yield on a Ribbed Bar
A370 distinguishes the yield point, the first stress below the maximum at which strain keeps increasing while stress does not, from the yield strength, the stress at a specified deviation from proportionality. A sharply yielding bar is read by the halt-of-the-force method, formerly the halt of the pointer or drop of the beam, or from the autographic diagram, and Delaware DOT still reads rebar yield by the halt of the pointer. A gradually yielding bar is read by the offset method: a line parallel to the elastic slope, offset by 0.2 percent strain, meets the curve at the yield strength. The older extension-under-load method records the stress at a specified total extension.
Most bar today yields sharply. Of about 200 A615 and A706 samples in Grades 60, 75 and 80 tested at one consulting laboratory between 2003 and 2013, fewer than 2 percent yielded gradually, while coiled bar never yielded sharply. Average actual yield ran 1.06 to 1.14 times the specified minimum, depending on grade. Bars of 100 ksi and above typically have no definite yield point, and cold working removes the plateau, so the offset method becomes normal as grades rise.
Extension under load has a long history in rebar. A615-68 used 0.5 percent for Grade 60, and ACI 318-71 required 0.35 percent for bars above 60 ksi. The 2008 and 2009 editions of A615 and A706 moved to the yield point or the 0.2 percent offset, and A615-09b, A706-09b and A615-12 also required a 0.35 percent check for some grades. In October 2013 ACI Committee 318 made the 0.2 percent offset the method for gradually yielding reinforcement in ACI 318-14. We treat the extension-under-load check as history; whether an order or an older specification still calls for it is read in that document.
For sharply yielding bar the method barely moves the number. On #5 bars tested at Oregon State University, the 0.2 percent offset and a 0.0035 extension-under-load reading gave 68.1 and 68.1 ksi for A615 Grade 60, 64.6 and 64.3 ksi for A706 Grade 60, 80.7 and 80.4 ksi for A615 Grade 80, and 86.2 and 85.4 ksi for A706 Grade 80. The A615 Grade 60 bar reached 102.2 ksi in tensile strength.
The offset method needs an extensometer; a sharply yielding bar can be read by the halt of the force and its elongation measured by hand, as Delaware DOT does. Where one is used, a coupler method proposed for AASHTO asks for ASTM E83 Class B2 or better. The UT Austin procedure extends a 50 mm extensometer to a 200 mm (7.874 in.) gauge, holds it with rubber bands or springs at about 600 g per knife edge, keeps the knife edges off the transverse ribs and removes it before fracture. Our extensometer guide covers the types.
Speed follows the distance between the grips. As the UT Austin procedure states the A370 rule, the crosshead moves at no more than 1/16 in. per minute per inch between the grips and no less than a tenth of that; that laboratory runs at 0.1 in./min. A 30 in. bar in 7 in. grips leaves 16 in., so the window is 0.1 to 1 in./min, about 2.5 to 25.4 mm/min. Delaware DOT adds: no faster than the load and the specimen can be properly observed.
Elongation and Where the Bar Breaks
Rebar elongation is measured over an 8 in. gauge length, and A370 allows it to be reported at a converted 200 mm gauge length. It depends on how it is measured and where the bar breaks.
Measuring After Fracture
Delaware DOT fits the broken ends together, measures between the gauge marks to the nearest 1/8 in., and reports the percentage increase with the original gauge length. That step is about 1.6 percentage points on an 8 in. gauge, against 2009-edition Grade 60 minimums of 7 to 9 percent, so the halves have to be fitted with care. NIST adds that the manual method excludes the elastic elongation while an extensometer reading includes it, so a report should say which was used.
Uniform elongation, the strain at peak stress before necking, is not required by A370 or the ASTM rebar specifications, as NIST noted in 2014, but it is useful in seismic design, and NIST suggests taking usable elongation as no more than 75 percent of it. A706-26a now has a uniform elongation annex that applies when supplementary requirement S1 is ordered. In mill data for #7 to #11 bars, mean total elongation was about 14.9 to 15.8 percent for A706 Grade 60 and 12.3 to 13.2 percent for A615 Grade 60.
When the Break Is in the Wrong Place
Delaware DOT treats break location as part of the result. If the fracture lies outside the middle half of the gauge length or in a punch mark, the elongation may not be representative: if it still meets the minimum it stands, and if not the test is discarded and repeated. The ACI Foundation draft treats a test as invalid when elongation is short and the fracture lies within 2 in. or two bar diameters of a grip. That draft is not A615, but a short elongation next to a jaw usually describes the grip, not the bar. Scale in the jaws, a vee insert outside the bar’s range, a bar off the axis and gauge marks punched too deep are the first things to check, and our article on why tensile specimens break outside the gauge section covers the general causes.
Sizing the Frame for the Bars You Test
The force follows from the nominal area and the minimum tensile strength. For Grade 60 at the 80 ksi minimum in force since A615-20, a #4 bar needs about 71 kN, a #8 about 281 kN, a #11 about 555 kN, a #14 about 801 kN and a #18 about 1,423 kN. Real bars break higher: the Oregon Grade 60 bar reached 102.2 ksi, about 28 percent above the minimum. Our own frame guidance is to take the area times the expected tensile strength and add 20 to 30 percent.
Our servo-hydraulic universal testing machine, the TM-SHM, comes in 300, 600, 1,000, 2,000 and 3,000 kN (67,400 to 674,400 lbf), with four columns up to 1,000 kN and six above. Its product page lists rebar among its typical applications and ASTM A370 among its standards. Force accuracy is ±0.5 percent at calibration Class 0.5 from 1 percent of full scale upward, and every model’s actuator speed range covers the 2.5 to 25.4 mm/min window above.
At the small end, a #3 Grade 60 bar yields at about 0.11 in.² times 60 ksi, or 29 kN, below the 30 kN that is 1 percent of a 3,000 kN frame and the bottom of its stated range. The UT Austin procedure notes that a large frame’s force error can matter for small bars, so a lower-capacity frame may serve them better. Jaw range is the second check: a #14, 43.0 mm nominal, fits the 30 to 55 mm round jaws of the 2,000 kN model; a #18, 57.3 mm, needs the 30 to 70 mm jaws of the 3,000 kN model; and a #11 at 35.8 mm sits just past the 35 mm top of the 1,000 kN model’s range. Ribs add to every diameter, so we confirm inserts for the bar measured over the ribs before quoting.
The frame also has to be verified where it is used. Our ASTM E4 page explains that force is verified against instruments calibrated to ASTM E74, commonly to ±1 percent of the reading, and that the lowest passing force sets the bottom of the verified range, which decides whether small bars on a large frame are covered at all.
Our calibration service verifies force, speed, displacement and extensometers through an A2LA-accredited ISO/IEC 17025 laboratory, and the TM-SHM package can include alignment per ASTM E1012 on request. Our article on calibration and certification services covers the subject in more depth.
Tension and compression spaces

Grip force rises with load
ISO/IEC 17025 calibration
Servo-Hydraulic Universal Testing Machine (300 kN – 3000 kN)Standards Compliance : ASTM E4, ASTM E8, ASTM F606, ASTM A370, ASTM E21, ASTM D3039, ISO 6892-1, ISO 6892-2, ISO 7500-1, ISO 527, ISO 9513, EN ISO...View machine →
Electro Mechanical Universal Testing System 50kN / 1000kN with Precision Load CellThe TM-EML Series D Dual Column Floor Standing Universal Testing System (50 kN – 1000 kN) by TensileMill CNC is a robust electromechanical solution...View machine →
Electro Mechanical Universal Testing System 5 kN / 50 kN with Precision Load CellThe TM-EML Series C - Dual-Column Benchtop and Floor-Standing Universal Testing System (5 kN - 50 kN) is an advanced electromechanical testing...View machine →