Composite Tensile Testing to ASTM D3039: Tabs, Wedge Grips and Load-Train Alignment

Composite laminates are some of the strongest materials a tensile laboratory sees, and some of the easiest to test badly. A unidirectional carbon coupon a millimeter thick can carry tens of kilonewtons, yet it can fail at the grip, split along its length, or report a modulus several percent off because one side of the coupon carried more strain than the other. Most of those failures are decided before the test starts: by how the coupon was cut, how the tabs were bonded, and how straight the load runs from the crosshead to the specimen.

ASTM D3039/D3039M is the test method most laboratories use for these materials. This guide follows a coupon through it: what the standard covers, why the specimen is a plain strip, how tabs and grips get the load in, how alignment is checked, and how strain and failure are read at the end.

What D3039 Covers

The current edition is D3039/D3039M-17, reapproved in 2025. It determines the in-plane tensile properties of polymer matrix composites reinforced by high-modulus fibers, with continuous or discontinuous fibers, in laminates that are balanced and symmetric with respect to the test direction. From one test it can give the ultimate tensile strength, the ultimate tensile strain, the tensile chord modulus, Poisson’s ratio and, for materials with a bilinear response, the transition strain. ASTM lists the uses as material specifications, research and development, quality assurance, and structural design and analysis.

The boundary with plastics testing is written into the plastics standard. ASTM D638 notes that resin-matrix composites reinforced with oriented continuous or discontinuous high-modulus fibers, above about 20 GPa, are tested to D3039 instead. A glass-filled molding compound is a D638 job. A carbon or glass fiber laminate is a D3039 job. The ISO counterparts split the same territory differently: ISO 527-5 covers unidirectional fiber-reinforced composites and ISO 527-4 covers isotropic and orthotropic ones such as fabrics, mats and multidirectional laminates.

The ASTM and ISO routes look alike, but they do not produce interchangeable numbers. The ISO 527-5 coupons sit close to the common D3039 sizes, 15 mm wide and 1 mm thick for 0 degree material and 25 mm wide and 2 mm thick for 90 degree material, sized so both types break at comparable forces and run in the same setup. ISO uses straight tabs, where D3039 also accepts beveled tabs, and the two methods determine some properties differently, including the strain interval for the modulus, so data qualified to one should not be relabeled as the other. The same tensile setup also serves ASTM D3518, which pulls a plus or minus 45 degree laminate to obtain in-plane shear stress, shear strain and shear chord modulus, so the same load train usually carries over to shear work.

ASTM is also clear about what moves the result. Among the factors a report has to record are the material and lay-up, specimen preparation, conditioning, environment, specimen alignment and gripping, and the speed of testing. Three of those happen at the test frame, and two happen before the coupon ever reaches it.

Is a fiber reinforced plastic tested to ASTM D638 or D3039?
It depends on the reinforcement. ASTM D638 sends resin-matrix composites reinforced with oriented continuous or discontinuous high-modulus fibers, above about 20 GPa, to D3039. A glass-filled molding compound is a D638 job, and a carbon or glass fiber laminate is a D3039 job. On the ISO side, unidirectional laminates go to ISO 527-5 and fabrics, mats and multidirectional laminates to ISO 527-4.

The Coupon: A Straight Strip and Its Tabs

A metal or plastic tensile specimen has a reduced gauge section so it breaks in the middle. A unidirectional composite cannot use that shape. The fibers run straight through the shoulder radius, and the laminate splits along them and fails at the transition instead of in the gauge. D3039 therefore uses a straight-sided coupon of constant cross-section, and gets the load into it through bonded tabs or a gripping surface that does not damage it.

Typical Coupon Sizes

The geometry depends on the lay-up, and the sizes commonly used with D3039 are consistent across testing laboratories and equipment makers. A 0 degree unidirectional coupon is typically 15 mm wide, 250 mm long and 1 mm thick, with tabs 56 mm long. A 90 degree unidirectional coupon is wider and thicker, 25 mm by 175 mm by 2 mm, with 25 mm tabs. Balanced, symmetric and random discontinuous laminates are typically 25 mm wide, 250 mm long and 2.5 mm thick, often without tabs. The widths are not arbitrary. A study of carbon fiber specimens trimmed with a diamond-coated cutter found no loss of properties on 12 mm wide coupons but a 10 percent loss on 6 mm wide ones, because the damaged edge made up a larger share of the section, and it noted the 25 mm width the standard recommends for balanced laminates as the way to keep edge damage from mattering.

How the load gets in
Tabs and Bevel on a 0 Degree Coupon
0 DEGREE COUPON, SIDE VIEW: LENGTH TO SCALE, THICKNESS EXAGGERATEDtab 56 mm, 1.5 mm thickbeveled tab end, about 7° (angle exaggerated)138 mm between tabs; 250 mm overall, 15 mm wide, 1 mm thickD3039 asks the grips to overhang the beveled part of the tab by about 10 to 15 mm when tabs are used.
The common 0 degree D3039 coupon drawn to scale along its length, with the thickness exaggerated: 56 mm glass fiber tabs with a beveled end of about 7 degrees, leaving 138 mm of laminate between the tabs. When tabs are used, D3039 asks the grip faces to overhang the beveled part of the tab by about 10 to 15 mm.
Scroll the diagram sideways to see all of it.

Tabs, Bevels and the Bond Line

Tabs spread the grip pressure so the jaws do not crush or notch the laminate. They are usually glass fiber laminate about 1.5 mm thick, bonded with a high-elongation adhesive in a thin, even bond line, and they must be the same thickness on both faces so the coupon sits on the grip centerline. The end of the tab can be straight or beveled. Practice in published research uses bevels around 7 degrees to reduce the stress concentration where the tab ends, and laboratory guidance pairs low-angle bevels with wedge grips and straight tabs with pressure-operated grips. D3039 itself asks that, when tabs are used, the grips overhang the beveled part of the tab by about 10 to 15 mm.

Aerospace qualification practice adds detail that saves failed tests. The FAA material qualification procedure asks for a tab adhesive that cures at or below the panel cure temperature, so bonding does not post-cure the laminate, for no peel ply on surfaces to be bonded, and allows the tabs to be ground flat after bonding if an uneven bond line would bend the specimen in the grips. Tabs are not mandatory for every laminate. Woven and multidirectional laminates often test well with an abrasive cloth between the jaws, while unidirectional coupons are where bonded tabs earn their cost, and 90 degree coupons are normally fitted with straight tabs.

Tabs bring risks of their own. An FAA survey of composite tension methods describes bonded tabs on straight-sided coupons as generally giving acceptable results, but notes that stress concentrations at the tab can make some results questionable and that hot, humid conditioning makes tab debonding more likely. Qualification programmes answer that with strain-compatible tab material, commonly glass or graphite woven fabric and a controlled bond line and tab thickness, so the tab does not become the weakest part of the coupon.

Does every composite tensile coupon need bonded tabs?
No. Woven and multidirectional laminates often test well with an abrasive cloth between the jaws, and balanced, symmetric and random discontinuous laminates are often tested without tabs. Unidirectional coupons are where bonded tabs earn their cost, and 90 degree coupons are normally fitted with straight tabs. Where tabs are used, keep them the same thickness on both faces.

Cutting the Coupon Without Damaging It

D3039 names poor fabrication, uncontrolled fiber alignment and damage from improper coupon machining as known causes of high data scatter in composites. Machining is the one of the three the testing laboratory controls. The FAA qualification procedure describes the usual route: coupons sectioned from panels with a water-cooled diamond saw, with care not to overheat the specimen and char the matrix, then surface ground to final dimensions, cut from the panel’s reference edge so the fiber direction stays within tolerance. NASA researchers preparing D3039 coupons cut them by waterjet and then inspected the cut areas ultrasonically for debonds before tabbing.

Heat is the hidden variable. The carbon fiber trimming study measured cutting temperatures of about 300 °C with a new tool and 475 °C with a worn one, far above the epoxy’s glass transition, and found that the worn tool smeared degraded resin over the cut face, which made the edge look smoother while hiding the damage under it. An edge that looks clean is not proof that it is sound. Angle-ply laminates add a further sensitivity: D3039 warns that edge softening in laminates with off-axis plies leads to premature failure and lower stiffness, and that strength and modulus of angle-ply laminates can be drastically underestimated. For quasi-isotropic laminates with a significant share of 0 degree plies, the standard notes that the effect is smaller.

Every coupon is measured after cutting, because the cross-section is what turns force into stress. A thickness reading 0.04 mm high on a 1 mm coupon understates strength by about 4 percent before the coupon is ever loaded. D3039 asks for measuring instruments accurate to within 1 percent of the dimension, typically about 0.0025 mm for thickness and 0.025 mm for width. The FAA qualification procedure builds a routine around that: at least two width and two thickness measurements in the gauge section of every specimen, one randomly selected specimen per subpanel checked against all dimensional tolerances, and small panels cut from a reference edge so the accumulated fiber direction error stays within 0.25 degrees. Spares belong in the same plan. The NASA team mentioned above fabricated additional panels to make sure at least five specimens were available for each series, and tabbed only the coupons that showed no edge defects in the scan.

TensileMill wedge clamping grips for composite and high-strength metal specimens
Wedge clamping grips. The wedge increases the holding force as the tensile load rises, which is why low-angle tab bevels are paired with this grip type.
Before a composite set goes to the frame
Cut cool and from the reference edge. Fiber angle and edge damage are set at the saw. A charred or fuzzy edge on a narrow coupon is a strength result you did not intend to measure.
Check the bond line. Equal tab thickness on both faces and an even adhesive layer keep the coupon on the grip centerline. Uneven tabs put bending in before the load does.
Measure thickness with the right anvil. D3039 calls for a ball-ended micrometer on an irregular bag-side surface and a flat anvil only when both faces are smooth.

Grips and Alignment: Getting the Load in Straight

D3039 asks for grips that apply enough lateral pressure to prevent slippage and notes that rotationally self-aligning grips are highly desirable to minimize bending. For wedge-action grips it describes lightly serrated faces, about one serration per millimeter, as satisfactory when kept clean and sharp, and warns that coarse serrations can cause grip failures on untabbed coupons. Smooth faces have also been used with hydraulic grips or an emery cloth interface. The standard reads a high percentage of grip failures, especially with high scatter, as a sign of a gripping problem rather than a material one.

Alignment is where composites are least forgiving. D3039 states that excessive bending causes premature failure and highly inaccurate modulus, and that bending can come from misaligned grips, a coupon installed off-center, or a coupon that is out of tolerance. It gives a target rather than a pass or fail line: good practice generally limits percent bending to about 3 to 5 percent at moderate strain levels, above 1000 microstrain, and a system showing more than the application tolerates should be readjusted.

The check itself uses an alignment coupon similar in size and stiffness to the specimens, with at least three strain gauges: two across the width on the front face and one on the back. Comparing the gauges separates bending in the thickness plane from bending in the width plane. The coupon is tested in four installations, as fitted, turned front to back, turned end for end, and both, so the bending that belongs to the machine can be separated from the bending caused by the coupon or the gauges. ASTM E1012 is the practice behind it, and alignment verification is a standing requirement in accredited aerospace laboratories. Our article on ISO, ASTM certification and NADCAP accreditation covers that side.

How bending is checked
Three Gauges, Four Installations
ALIGNMENT COUPON: WHERE THE GAUGES GO AND HOW IT IS INSTALLEDfront facegauges 1 and 2 across the widthback facegauge 3 on the centerline1 vs 2: bending across the width.Front vs back: bending through the thickness.FOUR INSTALLATIONS OF THE SAME COUPONas fittedturned frontto backturned endfor endbothturnsComparing the four separates the machine’s bending from the coupon’s.
D3039’s alignment check uses a coupon like the specimens with two gauges across the front face and one on the back. Testing it in four orientations separates the bending that belongs to the machine from the bending the coupon or the gauges bring.
Scroll the diagram sideways to see all of it.

How the check is run decides what it can find. D3039 recommends loading the alignment coupon until all three gauges read at least 500 microstrain in tension, with an average of at least 1000 microstrain, and allows bending to be examined during gripping, during loading, or both. Where to look follows the symptom: failures during gripping call for a check near the grip as it closes, modulus scatter for a check across the modulus range, and many breaks near the grips for a check near the grip at high load. E1012 alignment classes 5, 8 and 10 carry percent bending limits of 5, 8 and 10 percent, and whether to improve a frame further is left to agreement between the parties. Misalignment shows up as scatter, and scatter is paid for in larger batches of coupons. Once a system’s alignment has been verified, FAA qualification practice does not put back-to-back gauges on every specimen just to confirm percent bending.


Strain, Speed and Reading the Break

D3039 runs at a constant crosshead speed or strain rate chosen to break the coupon in roughly one to ten minutes, commonly 2 mm/min or a strain rate of 0.01 per minute. The modulus is a chord modulus over a fixed strain interval, commonly 1000 to 3000 microstrain, rather than the steepest part of the curve. Strain is measured with strain gauges or an extensometer. The 2017 text asks for an extensometer meeting at least ASTM E83 class B-1 over the strain range of interest, with a gauge length between 10 and 50 mm, and suggests class A for very stiff materials or transverse strain. Where modulus is wanted, it asks for strain on opposite faces of the coupon so bending can be corrected, and Poisson’s ratio needs a transverse measurement as well.

Strain gauges need their own care on composites. An active gauge length of 6 mm is recommended for most materials and it should not drop below 3 mm, while on woven laminates the gauge should be at least as long as the weave’s repeating unit. Surface preparation done the way it is for metals can cut into the matrix and damage the fibers beneath it, so the standard asks that reinforcing fibers are not exposed or damaged at the gauge site. Bonded gauges are not meant to measure to failure and a clip-on extensometer is normally taken off before the break, so video and other non-contact systems are used when strain at failure is needed.

Units deserve a line in the procedure. D3039 treats SI and inch-pound values each as standard on their own, notes that they are not exact equivalents, and warns that mixing the two can put a test out of conformance. Speed is the easy example. The commonly quoted rate is 2 mm/min, while its inch-pound counterpart, 0.05 in/min, is 1.27 mm/min, and NASA programmes testing to D3039 have run at 1.27 mm/min. Neither is wrong, but a report should state one system and keep the dimensions, the rate and the results in it.

At least five coupons are tested per condition, and every failure is recorded with a three-character code: the failure type, the area and the location. A 0 degree coupon that splits along its length in the gauge middle is coded SGM, a transverse coupon that breaks laterally in the gauge middle LGM, and explosive or edge-delamination failures in the gauge carry X or D as their first letter. Failures at or inside the tab, or within about one specimen width of the grip, are the ones laboratories commonly treat as invalid and replace, while explosive failures in straight 0 degree coupons are usually accepted when they start in the gauge section. Our guide on why tensile specimens break outside the gauge section explains the same logic for metal specimens.

Reading the result
Where It Broke and What the Code Says
READING THE THREE-CHARACTER FAILURE CODE ON A TABBED COUPONtabtabnear gripgauge section: top, middle, bottoma break here is a valid resultS G Mlong splitting, gauge, middletypical of 0 degree couponsL G Mlateral, gauge, middletypical of 90 degree couponsX G Mexplosive, gauge, middleD G Medge delamination, gauge, middle
The three characters record the failure type, the area and the location. Breaks in the gauge section are valid results; breaks at the tab or close to the grip are treated as invalid and the coupon is replaced. Only the code letters confirmed in open sources are shown.
Scroll the diagram sideways to see all of it.

A Worked Example: Strength, Chord Modulus and Frame Size

A published 0 degree carbon/epoxy example shows how the numbers fit together. The coupon is 15.0 mm wide and 1.0 mm thick, a 15 mm² section, and it fails at 33,000 N, so its ultimate tensile strength is 33,000 divided by 15, or 2,200 MPa. Between 1000 and 3000 microstrain the stress rises from 132 MPa to 396 MPa. The chord modulus is that rise, 264 MPa, divided by the strain interval of 0.002, which gives 132 GPa. If the curve stayed straight to the end, the coupon would break at about 1.7 percent strain, several times the strain at the top of the modulus window, which is why the modulus and the strain at failure are often measured in different ways.

Turning the curve into numbers
Strength and Chord Modulus, Step by Step
CHORD MODULUS ON THE WORKED EXAMPLE, 0 DEGREE CARBON/EPOXY01000200030004000strain, microstrain0132264396528MPamodulus window, 1000 to 3000396 MPa at 3000132 MPa at 1000run: 0.002rise: 264 MPaTHE ARITHMETIC33,000 N on 15 x 1.0 mm= 2,200 MPa strength264 MPa / 0.002= 132 GPa chord modulusTwo fixed points, not the steepesttangent. If the line stays straight,the break is near 16,700 microstrain.
A published 0 degree carbon/epoxy example: 33,000 N on a 15 by 1.0 mm section is 2,200 MPa, and the stress rise of 264 MPa across the commonly used 1000 to 3000 microstrain window, divided by 0.002, gives a chord modulus of 132 GPa. The line is drawn straight for clarity.
Scroll the diagram sideways to see all of it.

Capacity follows the laminate. A thin transverse coupon, 25 mm by 2 mm, breaks at about 2 to 3 kN, while the 15 mm by 1 mm carbon coupon above takes 33 kN, two thirds of a 50 kN frame, and thicker or wider laminates need more. A common way to size the frame is to multiply the expected strength by the cross-section and add a margin of 20 to 50 percent: a 1000 MPa laminate in a 15 mm by 2 mm coupon gives 30 kN, and a 30 percent margin takes it to 39 kN. Industry guidance treats 50 kN as normally enough for glass fiber laminates and 100 kN as often enough for carbon and glass. Size the frame and the load cell from the strongest coupon you expect, rather than from the average one. Our guide to choosing tensile grips and fixtures covers the grip side of that decision.

Composite testing equipment
Grips, Alignment and the Frame
Three parts of the load train decide whether a D3039 result belongs to the laminate: jaws that hold without crushing, a load train that stays straight, and a frame that measures strain on the coupon itself.
TensileMill composite testing fixture for carbon fiber and fiberglass laminates
Composite Testing Grips and Fixtures
Hydraulic wedge grips with surface-treated jaws hold carbon fiber and fiberglass laminates without crushing or slipping, alongside fixtures for compression, short-beam, V-notched and rail shear, and delamination tests. ASTM D3039, D3518, D7264 and ISO 527-4 and 527-5 are among the supported standards.
CFRP and fiberglass
Tension, shear, compression, delamination
Surface-treated jaws
TensileMill precision alignment device installed on a universal testing machine with a strain-gauged coupon
Precision Alignment Device
Installed between the crosshead and the grips, it adjusts load-train coaxiality with an integrated coaxiality meter, references ASTM E1012 and NASM 1312B, and retrofits to existing frames.
Load-train alignment
ASTM E1012 and NASM 1312B
Fits TensileMill and other frames
TensileMill TM-EML Series C dual-column universal testing machines
TM-EML Series C Universal Testing Machine
A dual-column frame from 5 to 50 kN with a 180 kN/mm frame stiffness, Class 0.5 force accuracy and six 24-bit analog channels for extensometer and strain gauge inputs, and the frame our ASTM D3039 page points to. Larger laminates move to the Series D frames up to 1000 kN.
5 to 50 kN
Six channels for strain inputs
Installation, training, calibration
Next step
Send us the laminate, the lay-up and the strongest coupon you test
Tell us the fiber and matrix, the lay-ups you test, the coupon widths and thicknesses, whether you tab your coupons, which standards your customers name, ASTM D3039, ISO 527-4 or ISO 527-5, and whether you need alignment verification for an accreditation. We will confirm the frame capacity, the grips, the alignment setup and the strain measurement for that work.
Related machines
Equipment That Does This Work

RELATED TO STANDARDS

More standards can be added on-site with licensed TM Software, no specialist training required.

Your team can extend the machine to new test standards at any time using the machine's licensed TM Software, without CNC programming experience or outside help.

Have a tensile sample prep or testing question?