Bolt and Fastener Tensile Tests to ASTM F606 and A370: Full-Size vs Machined Specimens

A bolt is one of the few products whose tensile test is usually run on the product itself. The finished bolt goes into the frame with its head, its thread and its coating, and the first number on the report is a load it has to reach. When the bolt is too large for the frame, or the order asks for elongation and reduction of area, a round specimen is turned from it instead, and the test starts measuring something different.

This guide follows both routes as ASTM F606/F606M and ASTM A370 frame them: the full-size tests, the stress area behind every published load, the machined specimen, and the fixtures and frame.

In short
What is the difference between a full-size and a machined bolt tensile test?
A full-size test pulls the finished bolt through its own head and thread and checks that it reaches a minimum load. With a wedge under the head it also tests the head-to-shank fillet. A specimen machined from the bolt gives the steel’s tensile strength, yield, elongation and reduction of area, but no longer loads the head, the fillet or the thread.

What ASTM F606 and A370 Cover

The current edition is ASTM F606/F606M-26a. It collects test methods for externally and internally threaded fasteners, washers, direct tension indicators and rivets. For bolts and screws it lists product hardness, proof load by three methods, axial tension and wedge tension of the full-size product, tension of machined test specimens, total extension at fracture, single shear and impact. For nuts it lists hardness, proof load and cone proof load.

The key line in the scope is about precedence. F606 is a set of methods; the product standard decides which tests apply and what the bolt has to achieve, and where the two differ, the product standard governs. A laboratory reads the bolt specification first. Units follow the same discipline: inch-pound and SI values are each standard on their own, inch values apply to inch fasteners and SI values to metric ones, and the two are not combined.

ASTM A370-26 covers mechanical testing of steel products and carries an annex for fasteners, and its product-specification-governs rule matches F606. Fastener test laboratories commonly cite F606/F606M and the fastener annex of A370 together.

On the metric side, ISO 898-1 sets property classes 4.6 to 12.9 for carbon and alloy steel bolts, screws and studs from M1.6 to M39. The class name is a formula: 8.8 means a nominal tensile strength of 800 MPa and a yield ratio of 0.8, so a nominal yield of 640 MPa.

The product specifications carry the numbers. ASTM F3125/F3125M consolidated the structural grades A325, A490, F1852 and F2280 and their metric versions into one specification for quenched and tempered bolts of 120 ksi (830 MPa) and 150 ksi (1040 MPa) minimum tensile strength, from 1/2 to 1-1/2 in. and M12 to M36. ASTM A307 covers carbon steel bolts and studs from 1/4 to 4 in., Grade A at 60 ksi minimum and Grade B between 60 and 100 ksi.


Full-Size Product or Machined Specimen

ISO 898-1 draws the line cleanly. A finished fastener has been through every manufacturing step and has not been machined into a test piece. A full-size fastener is a finished one whose shank is about equal to or larger than the thread diameter, or which is threaded to the head, or a fully threaded stud. A machined test piece is cut from a fastener to evaluate the material. Even the property names differ: elongation A and reduction of area Z belong to machined pieces, while full-size fasteners report elongation after fracture Af and Rpf, the stress at 0.0048d non-proportional elongation.

The full-size test comes first for a reason the RCSC Guide by Kulak, Fisher and Struik states plainly: bolt strength is specified by a tensile test of the threaded fastener, because the bolt’s load-elongation behavior matters more than the stress-strain curve of its steel, and the weakest section of a bolt in tension is the thread. The guide adds that ASTM requires a direct tension test of most sizes and lengths of full-size bolts.

Two specimens from one bolt
The Whole Bolt or the Steel Inside It
A. FULL-SIZE BOLTheadfilletshankthread, the weakest sectionB. ROUND SPECIMEN TURNED FROM THE SAME BOLTgauge4D (E8 inch) or 5D (metric practice)head, fillet and bolt thread are cut awayPosition and size inside the bolt: set by F606 and the product specification.What the result describesthe bolt as made: head, fillet, shankand thread loaded togetherTypical resultsminimum tensile load, wedge soundness,proof load; ISO 898-1: Af and RpfWhat the result describesthe steel inside the bolt, with thehead and the thread removedTypical resultstensile strength, 0.2 % offset yield,elongation, reduction of area;ISO 898-1: A and Z
A full-size test loads the head, the fillet, the shank and the thread together, with the thread as the weakest section. A round specimen turned from inside the same bolt removes all three features and measures the steel: tensile strength, 0.2 percent offset yield, elongation and reduction of area. Where the specimen sits in the bolt is set by F606 and the product specification.
Scroll the diagram sideways to see all of it.

A machined specimen answers other questions: tensile strength, 0.2 percent offset yield, elongation and reduction of area of the steel inside the bolt. F606 includes it as a method of its own, and some bolts leave no choice: when a large bolt’s minimum breaking load is beyond the frame, a turned specimen is the practical test. The RCSC Guide itself shows stress-strain curves from 0.505 in. specimens turned from full-size A325 and A490 bolts.

Round machined tensile specimens with shouldered ends laid out on a table
Round machined specimens. A specimen turned from a bolt tests the steel inside it, and no longer loads the head, the fillet or the thread.

The current product specification and F606 decide which route applies; the rules have moved over the years. In the A325 and A490 specifications of the mid-1980s, as the RCSC Guide describes them, larger bolts could be tested with machined specimens and bolts shorter than three diameters only had to meet hardness limits. NASA-STD-8739.14 notes that fasteners smaller than #10 or shorter than two diameters may not be testable at receiving inspection, so they may have to come from a qualified supplier with full traceability.

Full-size bolt
Loads: head, fillet, shank and thread together
Reports: minimum tensile load, wedge soundness, proof load
ISO 898-1 names: Af and Rpf
Machined specimen
Loads: the steel, with head and thread cut away
Reports: tensile strength, 0.2 % yield, elongation, reduction of area
ISO 898-1 names: A and Z

The Three Full-Size Tests

Acceptance testing of finished bolts comes down to three pulls on the whole product: axial tension to a minimum load, the same pull with a wedge under the head, and a proof load that the bolt must carry without stretching permanently.

Axial Tension of the Finished Bolt

The bolt is held by its thread in a threaded fixture and by its head, then pulled to fracture. It passes if it carries at least the minimum tensile load for its size, grade and thread series and breaks in the body or the thread, not at the junction of head and shank; industry summaries of F606, SAE J429 and ISO 898-1 agree on that location rule. Fastener makers commonly cite a crosshead speed of no more than 1 in./min (25 mm/min) for full-size tensile and wedge tests.

The result is not an installation capacity. In tests the RCSC Guide reports, bolts torqued to failure lost 5 to 25 percent of their ultimate strength, 15 percent on average, while bolts preloaded by torquing and then pulled in direct tension lost nothing significant.

Wedge Tension and the Head-to-Shank Fillet

In a wedge test a hardened wedge with an inclined face sits under the head of a hex or square head bolt or a socket head cap screw. The head is loaded obliquely, so the fillet under it sees bending on top of tension. The bolt still has to reach its minimum tensile load and break in the body or thread, which shows that head and fillet are sound and ductile. Fastener makers commonly specify a wedge hardened to at least 45 HRC.

How the wedge test loads the head
A Head on a 10 Degree Slope
SIDE SECTION, WEDGE AT A TRUE 10 DEGREES, BOLT PROPORTIONS SCHEMATICpullhorizontalhardened wedge, top atthe wedge anglefixed platefree thread betweenshank and fixturethreaded fixtureengages the bolthead-to-shank fillet:tension plus bendingone side of the headbears first on the slopeWHAT THE WEDGE ADDSAxial test: the head seats flat andthe bolt sees straight tension.Wedge test: the head seats on a slope,so the fillet under it bends as well.Wedge angle, A325 bolts10° for 1/4 to 1 in.6° over 1 in. (FHWA checklist)Passthe minimum tensile load is reachedand the break is in the body or thethread, not at the filletFor a 1 in. A325 bolt the FHWA wedgeminimum is 72,700 lb: the fullminimum tensile load, not a reduced one.
The bolt is pulled through a threaded fixture while its head sits on a hardened wedge, so one side of the head bears first and the head-to-shank fillet bends as well as stretches. For A325 bolts the FHWA checklist sets 10 degrees up to 1 in. and 6 degrees above. The bolt must still reach its full minimum tensile load and break in the body or thread.
Scroll the diagram sideways to see all of it.

For A325 bolts the FHWA inspection checklist sets the wedge angle at 10° for 1/4 to 1 in. and 6° over 1 in., with no head or shank fracture allowed, and a minimum wedge load of 72,700 lb at 1 in. Divide that by the 0.606 in.² stress area of a 1-8 thread and the result is 120 ksi, the full A325 minimum: the wedge test is not run at a reduced load. A 1992 FHWA supplemental specification required wedge tests on full-size bolts, after galvanizing for galvanized bolts. ISO 898-1 requires “no fracture” in head soundness for every class.

Proof Load, on the Bolt and on the Nut

The proof load is the tension a fastener must carry without evidence of permanent deformation, about equivalent, in the RCSC Guide’s words, to the bolt’s yield or 0.2 percent offset load. In the length-measurement method the bolt is measured, loaded to proof and released, and measured again; the FHWA checklist allows a change of ±0.0005 in. Its A325 proof load at 1 in. is 51,500 lb, 85 ksi on 0.606 in.². ISO 898-1 gives stress under proof load instead: 580 MPa for class 8.8 up to 16 mm and 600 MPa above, 830 MPa for 10.9 and 970 MPa for 12.9, so an M20 class 8.8 bolt has a proof load of 147,000 N.

Bolt, nut and the proof load test
Three Loads on One 1 In. Assembly
1 IN. A325 BOLT AND BLACK NUT, FHWA CHECKLIST VALUES020406080100load, thousand lbbolt proof load51,500 lb = 85 ksi on 0.606 in.²bolt minimum tensile load72,700 lb = 120 ksinut proof load87,250 lbThe nut is rated above the bolt’s breaking load, so a sound assembly fails by bolt fracture, not by stripping.PROOF LOAD BY LENGTH MEASUREMENT1Measure length L0between the same two points2Apply the proof loadin direct tension, then release3Measure length L1with the same setup4CompareL1 − L0 within ±0.0005 in.A permanent stretch beyond that limit means the bolt yielded below its proof load.
FHWA checklist values for a 1 in. A325 bolt and black nut: the bolt proof load sits below the bolt’s minimum tensile load, and the nut proof load sits above it, so a sound assembly breaks the bolt instead of stripping the nut. Below, the proof test by length measurement, which allows a change of 0.0005 in. either way.
Scroll the diagram sideways to see all of it.

Nuts are proof tested on a hardened threaded mandrel, as our threaded fastener grips page describes: the nut is installed on the mandrel and loaded to the specified tension to confirm its threads carry it without stripping. In the FHWA table every nut proof load sits above the matching bolt’s minimum tensile load, 87,250 lb against 72,700 lb at 1 in. The RCSC Guide gives the reason: a bolt fracture is easy to see, while stripping can develop with an imperceptible drop in torque, so nuts are specified stronger than their bolts.


Stress Area: Where Every Published Load Comes From

Bolt acceptance is written in loads because a thread has no single diameter. The load is calculated on the tensile stress area, which for inch threads is 0.7854 (D − 0.9743/n)², with D the nominal diameter in inches and n the threads per inch. The metric form uses the mean of the pitch diameter d2 and the minor diameter d3 as the diameter of an equivalent plain round.

The area behind the published loads
Tensile Stress Area of a Thread
M20 x 2.5 HALF SECTION, RADIAL SCALE TRUE, AXIAL SCALE x 0.6equivalent plain round(toward the bolt axis)major diameter d = 20 mmpitch diameter d2 = 18.376 mm(d2 + d3)/2 = 17.655 mmminor diameter d3 = 16.933 mmTHE AREA EVERY LOAD IS BUILT ONMetricAs = 0.7854 ((d2 + d3)/2)²M20 x 2.5: 244.8 mm², table value 245x 830 MPa = 203 kN, the ISO 898-1minimum load for M20 class 8.8Inch, D in in., n threads per inchAs = 0.7854 (D − 0.9743/n)²1-8: 0.606 in.²x 120 ksi = 72,700 lb, the FHWAminimum for a 1 in. A325 boltAbout 75 % of the nominal bolt area (RCSC 2020).
A thread has no single diameter, so its load is calculated on an equivalent plain round whose diameter is the mean of the pitch and minor diameters. For M20 x 2.5 that gives 245 mm², and for a 1-8 inch thread 0.606 in.². Multiplied by the minimum tensile strength, each area reproduces the published minimum load.
Scroll the diagram sideways to see all of it.

Worked through, the formula reproduces the published tables. A 1-8 bolt has 0.606 in.², a 7/8-9 bolt 0.462 in.² and a 1-1/2-6 bolt 1.405 in.². An M20 x 2.5 thread gives d2 = 18.376 mm and d3 = 16.933 mm, a mean of 17.655 mm and 244.8 mm², tabulated in ISO 898-1 as 245 mm². Times the 830 MPa class 8.8 minimum above 16 mm, that is the 203,000 N minimum ultimate load ISO 898-1 lists for M20 in 8.8.

A tensile strength reported for a full-size bolt is the breaking load divided by the stress area, not the shank or nominal area; RCSC notes that for the usual structural sizes the stress area is about 75 percent of the nominal area. And the area belongs to the thread form: NASA’s fastener design manual, RP-1228, notes that UNJ threads, with a larger root radius, have a larger minor diameter and net tensile area than UNC or UNF threads of the same size.

0.606 in.²
stress area of a 1-8 bolt thread
72,700 lb
FHWA wedge minimum for a 1 in. A325 bolt, exactly 120 ksi on that area
245 mm²
stress area of an M20 x 2.5 thread in ISO 898-1

Turning a Specimen From a Bolt

Where the specimen is taken from inside the bolt and how large it is turned are set by F606 and the product specification; check those clauses in the edition your order names. The ASTM E8 standard round is 0.500 in. (12.5 mm) in diameter with a 2 in. (50 mm) gauge length, a 4D proportion, while metric practice commonly uses 5D. Elongation depends on that gauge length, so the result is reported with its convention, and it is not interchangeable with the full-size Af.

The bolt’s hardness decides the lathe. ISO 898-1 puts class 10.9 at 32 to 39 HRC and 12.9 at 39 to 44 HRC, and RCSC’s 2020 specification gives Grade A490 a 38 HRC maximum. Our TensileTurn CNC Classic Upgrade turns stock up to 2 in. (51 mm) in diameter and 16 in. (406 mm) long in material up to 55 HRC, which covers those classes, into standard, sub-size, threaded and button-head specimens. The TensileTurn CNC Industrial Upgrade, with an 8 in. swing and a 4 in. chuck, also makes threaded and button-head specimens, and the TensileTurn CNC XL, with a 300 mm turning diameter and 550 mm turning length, takes larger blanks.

The ends have to suit the grips that will pull the specimen. As our article on threaded tensile specimens explains, the thread on a machined specimen must match the thread of the tester’s grips in diameter and length.

Our guide to preparing tensile specimens to ASTM A370 lists what to record with every specimen: the product form and specimen type, the position in the product, how the blank was removed and how much stock came off, the program used, and the measured, not nominal, reduced-section diameter. For a bolt, the product form means its grade, size and lot.

Before a specimen turned from a bolt goes to the frame
Keep the bolt’s identity. Grade marking, size, thread and lot travel with the specimen.
Match the ends to the grips. The specimen’s end thread follows the grip thread, not the bolt’s own thread.
Report the convention. Use the measured diameter for the stress and state whether elongation is over 4D or 5D.

Fixtures, Frame Capacity and Alignment

A full-size bolt is held by its own features. Our threaded fastener grips use threaded adapters that engage the part’s thread instead of clamping the outside, with interchangeable inserts for different thread sizes and capacities often exceeding 100 kN. As our guide on how to choose tensile test grips and fixtures points out, threaded ends are seated in a matching fixture, not clamped, and ordering grips without checking the end style is a common mistake.

How much thread sits in the fixture changes the result. A 1992 paper by FHWA and AISC engineers warns that stripping can occur with only a few threads in the grip, that three to five complete threads are desirable, and that bolts with more threads in the grip show more ductility and a lower apparent tensile strength. Fastener makers commonly specify six full threads exposed between the grips, four on heavy hex structural bolts.

Capacity follows from the stress area. ISO 898-1 minimum ultimate loads put an M20 class 8.8 bolt at 203,000 N and an M30 in 10.9 at 583,000 N, both within a 1,000 kN frame, while an M36 needs 1,020,000 N in 10.9 and 1,200,000 N in 12.9, the 2,000 kN class. A 1-1/2 in. F3125 Grade A490 bolt at 150 ksi on 1.405 in.² needs about 211,000 lbf, or 938 kN, at the minimum. Real bolts break higher: in historical data the RCSC Guide reports, A490 bolts exceeded their minimum by 10 percent on average, which takes that bolt to about 1,030 kN, just past a 1,000 kN frame.

Our servo-hydraulic universal testing machine, the TM-SHM, comes in 300, 600, 1,000, 2,000 and 3,000 kN. Its page lists ASTM F606 and A370 among its standards and bolts, nuts and studs among its specimens, with Class 0.5 force accuracy of ±0.5 percent from 1 to 100 percent of full scale. Its round-jaw ranges are for bars, so bolts are quoted with threaded fixtures sized to the thread. Our hydraulic UTM grips and fixtures include proof load fixtures for fasteners, with the nut-proof setup on a hardened threaded mandrel, for loads in the hundreds of kilonewtons, and our dual-action hydraulic wedge grips, which name bolts among their specimens, work in side-action or wedge-action mode.

Off-axis loading at high force introduces bending, which on a bolt adds to what the head and thread already concentrate. Load-train alignment is checked to ASTM E1012; our precision alignment device does that on our electromechanical frames from 50 to 600 kN. Force is verified to ASTM E4 over the range your smallest and largest bolts use.


Reading the Break and Writing the Report

A bolt that breaks in the free thread or the body has behaved as designed. A break at the head-to-shank fillet fails the test at any load, because it points to a fault at the fillet or a material too brittle for bending. A published industry case names folds from cold heading, too small an under-head radius, quench cracks and wrong material or tempering as the usual causes, and adds a lesson in sampling: an A307 lot passed the required three-piece wedge test, yet folds in a small percentage of parts appeared only when two laboratories tested samples of 20, and the replacement claim passed $2,000,000. The recommended response to a head-shank complaint is to quarantine the lot and test a much larger sample.

Does a head-to-shank break fail a bolt that reached its minimum load?
Yes. Industry summaries of F606, SAE J429 and ISO 898-1 require the fracture to be in the body or the thread. Fastener makers note one exception: screws threaded to the head, where a break that starts in the thread may run into the fillet before separation. Record where the break started, not only where it ended.

Stripped threads are a different finding: they say the engagement, the mating thread or the nut was the weak link, not the bolt. RCSC’s 2020 specification describes a common cause on galvanized assemblies: nuts are overtapped to clear the coating, which reduces engagement and stripping strength, and only A563 DH and DH3 and A194 2H nuts keep enough strength to serve as galvanized nuts. The FHWA checklist requires physical tests on galvanized fasteners after galvanizing. For machined rounds, see our article on why tensile specimens break outside the gauge section.

The report has to let a reader repeat the decision. NASA-STD-8739.14 asks for the break location, the ultimate load or strength, and the specification minimum and maximum. The FHWA checklist expects a certified report for structural bolts to carry the mill heat number, the lot number, and proof load, wedge tensile, hardness and coating results for the bolts, proof load and hardness for the nuts and hardness for the washers. For a machined specimen, add the drawing, the measured diameter and the gauge-length convention.

Fastener testing equipment
Full-Size Bolts and Specimens Turned From Them
A frame sized for your strongest bolt with a margin, fixtures that load the bolt through its own thread, and a lathe that turns a hardened bolt into a round specimen.
Servo-Hydraulic Universal Testing Machine
The TM-SHM runs from 300 to 3,000 kN at Class 0.5 and lists ASTM F606 and A370 among its standards, with bolts, nuts and studs among its specimens.
300 to 3,000 kN
±0.5 percent force accuracy
1 to 100 percent of full scale
Threaded Fastener Grips
Threaded adapters that engage the fastener’s own thread, interchangeable inserts for different thread sizes, and the nut-proof setup on a hardened threaded mandrel, for tests to ASTM F606.
Bolts, studs and nuts
Often exceeding 100 kN
Hydraulic fixtures for higher loads
TensileTurn CNC Classic Upgrade
Turns round, sub-size, threaded and button-head specimens from stock up to 2 in. (51 mm) in diameter and 16 in. long, in material up to 55 HRC.
Specimens from bolts
Up to 55 HRC
Threaded and button-head ends
Next step
Send us your bolt sizes, grades and the tests your orders name
Tell us the smallest and largest fasteners you test, their grades and threads, the tests your specifications call for (axial, wedge, proof load, nut proof or machined specimens), and how many parts a shift runs. We will confirm the frame capacity with a margin over your strongest bolt, the threaded fixtures for your sizes, and, if you machine specimens, the lathe and the specimen ends that match your grips.
Related machines
Equipment That Does This Work

RELATED TO STANDARDS

More standards can be added on-site with licensed TM Software, no specialist training required.

Your team can extend the machine to new test standards at any time using the machine's licensed TM Software, without CNC programming experience or outside help.

Have a tensile sample prep or testing question?